Manganese spinel ferrite (MnFe2O4) thin films were deposited by Pulsed Laser Deposition (PLD) at different temperatures to study the effect of growth conditions on their structural, thermoelectric and magnetic properties of the samples. X-ray diffraction reveals a progressive increase of crystallinity and a preferential orientation along the [311] direction of the spinel structure with increasing deposition temperature. The thin films, with an average thickness of similar to 180 nm, show in-plane isotropic reduced remanent magnetization, (M-r/M-max), whereas both the M-r/M-max and coercivity (H-C) are systematically lower in the out-of-plane direction. These magnetic parameters strongly depend on the deposition temperature, reaching maximum values of M-r/M-max similar to 0.7 and H-C similar to 0.4 kOe for films grown at 773 K. Thermoelectric measurements show a negative Seebeck coefficient (S) over the investigated temperature range (313-613 K), consistent with n-type conduction. The Seebeck coefficient remains relatively stable with temperature, varying from -3 & micro;V/K to -180 & micro;V/K across the series, while the electrical conductivity (sigma) increases from 0.1 S/m to about 1 S/m with increasing temperature. Both quantities are strongly affected by the deposition temperature, resulting in a maximum calculated power factor (PF) of 0.07 & micro;W/(m & centerdot;K-2) at 613 K for the film deposited at 473 K. These results are promising for the development of multifunctional materials with both magnetic and thermoelectric properties that can be tailored through different deposition temperatures.
Effect of the deposition temperature on the properties of MnFe2O4 thin films
Giribaldi A.;Maltoni P.;Piscino C.;Peddis D.;Artini C.;Mele P.
2026-01-01
Abstract
Manganese spinel ferrite (MnFe2O4) thin films were deposited by Pulsed Laser Deposition (PLD) at different temperatures to study the effect of growth conditions on their structural, thermoelectric and magnetic properties of the samples. X-ray diffraction reveals a progressive increase of crystallinity and a preferential orientation along the [311] direction of the spinel structure with increasing deposition temperature. The thin films, with an average thickness of similar to 180 nm, show in-plane isotropic reduced remanent magnetization, (M-r/M-max), whereas both the M-r/M-max and coercivity (H-C) are systematically lower in the out-of-plane direction. These magnetic parameters strongly depend on the deposition temperature, reaching maximum values of M-r/M-max similar to 0.7 and H-C similar to 0.4 kOe for films grown at 773 K. Thermoelectric measurements show a negative Seebeck coefficient (S) over the investigated temperature range (313-613 K), consistent with n-type conduction. The Seebeck coefficient remains relatively stable with temperature, varying from -3 & micro;V/K to -180 & micro;V/K across the series, while the electrical conductivity (sigma) increases from 0.1 S/m to about 1 S/m with increasing temperature. Both quantities are strongly affected by the deposition temperature, resulting in a maximum calculated power factor (PF) of 0.07 & micro;W/(m & centerdot;K-2) at 613 K for the film deposited at 473 K. These results are promising for the development of multifunctional materials with both magnetic and thermoelectric properties that can be tailored through different deposition temperatures.I documenti in IRIS sono protetti da copyright e tutti i diritti sono riservati, salvo diversa indicazione.